An air-handling cabinet maker in Saudi Arabia sent us a door panel and a complaint: the stiffeners welded to the inside of it were pulling the face out of flat, and the welds themselves were inconsistent from one stiffener to the next. Same sheet, same coating, same operator.

We spent two days on their floor with a 3000 W boom laser and a marker pen. What came out of it is the sheet in the photograph, and the numbers on it are not the ones we expected to write.

latest company news about Six Stiffeners, One Panel: Setting Up a Galvanised Cabinet Weld  0

The trial panel on the customer's bench, with the stiffeners laid out and the setting for each joint written on the sheet by hand. Six lengths, two power figures, and a tick beside every weld that passed.

One Panel, Six Lengths

The panel is 1.0 mm galvanised, and it carries folded stiffeners at six lengths between 900 mm and 1500 mm, plus a few short ones near the edges. The grade, the coating and the thickness are identical at every joint. Each joint still needed its own setting.

The reason is that a stiffener is not a flat lap. It is a folded section with a flange standing off the sheet, and it behaves like a fin: heat leaves the weld by running along the stiffener instead of spreading sideways into the panel. A 1500 mm stiffener carries heat away faster than a 900 mm one, and the joint that is easiest to weld is not the one you would guess.

What the Marker Wrote Down

Beside each joint there is a power figure and a verdict: 2500 W, 2000 W, and "set ok" ticked next to the ones that held. Two settings across six lengths, and the split does not follow the length in a straight line.

That is the whole value of a trial like this. Nothing in the drawing predicts which joint needs which number, so you run the panel, you write the number on the sheet, and the sheet goes back to the machine as a program. It does not go into somebody's memory, which is where the previous settings had been living.

Where Galvanised Punishes You

Zinc boils far below the temperature at which steel melts, and under a laser it does it in a fraction of a second. The coating vaporises out of the joint and pushes back; if the fit-up is loose, the vapour has somewhere to go and leaves a porous, undercut seam that looks welded and is not.

Three things control that, in order: the gap under the stiffener, the shielding gas, and the speed. A stiffener bowed by 0.2 mm along its length will weld at one end and fail at the other, which is exactly how a panel acquires an intermittent seam that nobody can explain afterwards. The fixture therefore does more work than the laser does. On this panel the stiffeners are clamped down before the weld starts, and the clamps are the reason the same program behaves the same way on Friday as it did on Monday.

latest company news about Six Stiffeners, One Panel: Setting Up a Galvanised Cabinet Weld  1

A finished door panel, stiffeners welded from the inside. The seam is intermittent on purpose: longer stitches would pull the face out of flat.

The Distortion Is a Separate Problem

The welds that held were also pulling the face out of flat, and that is not a welding fault, it is a heat-input budget. There are two ways to spend less: fewer, longer stitches, or a sequence that jumps between stiffeners so the panel is never hot in one place. The second costs nothing and is what we ended up using.

What to Ask Before You Approve the Sample

  • Can I see the setting for every joint, written down, or only the setting for the sample that was welded in front of me?
  • What is the permitted gap under the stiffener, and who checks it — the welder or the fitter?
  • How flat does the face have to be after welding, and is that measured, or eyeballed against a straight edge?

A cabinet door that is 2 mm out of flat will still close. It will also show a shadow line under a downlight, and that is the part the end customer sees. It is cheaper to settle that on the bench with a marker pen than on site with a service call.

PDKJ continues to provide customized laser welding and resistance welding solutions based on different materials, workpiece structures, welding requirements, and production applications.

Related Products

latest company news about Six Stiffeners, One Panel: Setting Up a Galvanised Cabinet Weld  2

Our shop floor in Dongguan. Trials like the one in this article are run here first, on the customer's parts, before anyone travels.

Contact PDKJ

Send us your part drawing or a sample, and our engineers will run a welding feasibility trial on your own material and recommend the equipment configured for your application.