The Schedule Nobody Uses: Preheat, Up-Slope And Post-Heat
2026/11/16
The Schedule Nobody Uses: Preheat, Up-Slope and Post-Heat
Almost every resistance welding controller on the market offers eight or nine segments in a schedule, and almost every shop uses three of them: squeeze, weld, hold. The rest — preheat, up-slope, multiple impulses, down-slope, post-heat — sit in the menu unused, because nobody was taught what they are for and the machine welds without them.
On mild steel, at 1 to 2 mm, that is a reasonable position. On a 4 mm stack, on coated material, on high-strength or high-carbon steel, the unused segments are the difference between a joint that passes and a joint that cracks in the customer's store.

Stamped high-strength steel parts on a fixture table, waiting to be welded. On this class of material the schedule matters as much as the current, because what happens after the nugget forms decides whether the joint cracks.
A Schedule Is a Sequence, Not a Number
The three settings everybody knows are the middle of a longer sentence. Squeeze brings the electrodes to force before any current flows. Weld is the current that makes the nugget. Hold keeps the force on while the nugget solidifies under pressure — take the force off too early and a sound nugget tears itself apart as it shrinks.
The segments that get skipped sit on either side of those three. Before them, preheat and up-slope decide how the metal arrives at welding temperature. After them, down-slope, post-heat and a second hold decide how it leaves. Each is measured in cycles, and at 50 Hz one cycle is 20 milliseconds, so the whole sequence is usually over in under a second.
That brevity is why the segments feel optional. Nothing in the finished part announces whether it was welded in one step or five, and the difference only shows up later, in the tests nobody runs on a Tuesday.
Preheat: Buying Tolerance With Time
Preheat is a low current passed through the stack before the welding current arrives. It does two things. It drives out surface contamination and levels the contact resistance across the joint, which is why a stack that expels at the start of the weld often stops expelling once a preheat pulse is added. And it warms the surrounding metal, so the welding current has less cold steel to heat before the nugget can grow.
The cases where it earns its keep are predictable: thick stacks of three sheets or more, heavily coated material, and parts that arrive cold from an unheated store in winter. The cost is time — a preheat of ten to twenty cycles is added to every weld, and at 40 welds a minute that is a real number. It is still cheaper than a 20 percent expulsion rate, which is what it usually replaces.
Up-Slope and Down-Slope: The Two Ramps
Up-slope ramps the current from a low value to the welding value over a few cycles instead of switching it on at full amplitude. Its job is to stop the first instant of the weld from exploding: at cold contact resistance the same current that is correct two cycles later is far too much at the beginning, and the result is a small ejection of molten metal and a welded-in crater.
Down-slope does the reverse at the end, and its job is metallurgical rather than electrical. A nugget that is quenched from welding temperature by cold electrodes and cold sheet forms martensite in the heat-affected zone, and martensite is hard, brittle and prone to cracking. Ramping the current down over five or ten cycles slows the cooling enough to change what forms. On mild steel this is a nicety. On high-carbon steel and on some advanced high-strength grades it is the difference between a weld and a delayed crack.
Post-Heat: The Segment Nobody Believes In
Post-heat is a second, much lower current applied after the nugget has formed, while the electrodes are still under force. It does not add strength to the nugget. It tempers the metal immediately around it, which is where cracking starts.
The resistance to using it is always the same argument: the part looks fine, the peel test passes, and the segment costs time. The counter-argument is that a delayed crack does not appear in a peel test either. It appears a day later, or after the part has been painted and baked, at which point the whole batch is suspect. On boron steels and on anything with a carbon equivalent above about 0.3, we now put post-heat in the schedule by default and take it out only if the customer has data showing they do not need it.

A stainless bracket with two spot welds through a strip. Both marks are clean; the question a schedule cannot answer from the surface is what the metal around them did on cooling.
Multiple Impulses: Stepping the Nugget Up
Instead of one long weld, the schedule can fire two or three shorter impulses separated by cooling cycles. Each impulse grows the nugget a step, and the pause between them lets the heat spread sideways rather than straight up into the electrode. On thick stacks this reduces both expulsion and electrode wear. On coated material it gives the coating time to be pushed out of the interface instead of being trapped in the nugget.
The penalty is that the total weld time goes up for the same nugget, so a line balanced on cycle time will notice. It is worth noticing: a line that is 8 percent slower and does not stop for tip changes every two hours is usually the faster line by Friday.
Where It Goes Wrong in Practice
The first failure is copying a schedule. A number that works on 1.5 mm cold-rolled steel is applied to 1.5 mm galvanised, and the only thing that changes is the electrode life and the expulsion rate. The second is a controller with coarse resolution: if the shortest weld time the box can deliver is five cycles, thin sheet has no schedule at all, only a choice of whether to burn through. The third is the habit of tuning only the weld current, which is the one variable that cannot fix a cooling problem or a fit-up problem.
The fourth is documentation. A schedule that exists only as numbers in a controller is lost the first time the controller is replaced, and the replacement is always set up by somebody who was told "about the same as before".
What to Ask For
When a supplier hands over a machine, the schedule should come with it in writing — every segment, in cycles, with the material and thickness it was proven on. That document is worth more than the parameter printout, because it records intent rather than a snapshot.
| Segment | What it does | When it earns its keep | What it costs |
|---|---|---|---|
| Preheat | Levels contact resistance, warms the stack | Thick stacks, heavy coating, cold store | Time per weld |
| Up-slope | Ramps current in, prevents start expulsion | Coated and oxidised surfaces | Two to five cycles |
| Multiple impulses | Grows the nugget in steps, spreads heat | Thick stacks, coated steel | Weld time, and cycle balance |
| Down-slope | Slows the cooling through the transformation | High-carbon and HSLA grades | Five to ten cycles |
| Post-heat | Tempering pulse under force | Crack-sensitive steels | Time, and the argument |
None of these segments make a bad joint good. They make a marginal joint repeatable, and repeatability is the only thing a production line is actually buying.
PDKJ continues to provide customized laser welding and resistance welding solutions based on different materials, workpiece structures, welding requirements, and production applications.
Related Products

The finished-goods area in Dongguan. Every machine leaves with its schedules written down, not left in the controller as a set of numbers nobody can explain.
Contact PDKJ
Send us your part drawing or a sample, and our engineers will run a welding feasibility trial on your own material and recommend the equipment configured for your application.
WhatsApp: +86 136 1279 3248
Email: jay@gd-pw.com
Website: https://www.spotlaserwelding.com/contactus.html
Address: 1-2F, Building 3, Qichen Industrial Park, No. 26 Luxi 1st Road, Liaobu Town, Dongguan City, Guangdong Province, China